Activated carbon is routinely used as part of the gold recovery process at many mines around the world. Activated carbon is used in both carbon in leach (CIL) and carbon in pulp (CIP) techniques. These CIL and CIP techniques recover gold (Au) from pulp or solutions derived from the cyanidation process. According to the World Gold Council, more gold is recovered from cyanidation than any other process.

Gold cyanidation is a hydrometallurgical process that extracts gold from ore by converting the gold to a water-soluble coordination complex. Activated carbon adsorbs the gold from the resulting solution. The carbon is then stripped of the gold before being passed through an electrowinning circuit and smelted to produce gold bars.

Monitoring the content of gold and other elements within the activated carbon enables process optimization and maximum gold recovery. The Vanta™ portable XRF analyzer is used as a replacement for traditional laboratory techniques within the mine-site laboratory due to its speed, ease of use, and significantly improved accuracy and precision.

The Vanta analyzer provides accurate chemistry for more than 30 elements in solids and liquids, from trace level to percent level, from samples across the entire minerals cycle. The Vanta analyzer can be used to measure the gold loading of activated carbon from each of the tanks used as part of the process either in unprepared coarse form or after undergoing a fine grind.

Gold concentrations within activated carbon cover a wide range, often measuring as high as 10,000 grams/ton (g/t), or 1%. The Vanta analyzer is used to monitor silver (Ag), copper (Cu), and calcium (Ca) within carbon from various mine sites.

Monitoring calcium within activated carbon is useful. Lime is used as part of the cyanidation process, and repeated exposure to lime dosages blocks the pore spaces in activated carbon, reducing the carbon’s ability to extract gold. When too much calcium is detected, it is an indicator that new carbon is necessary or that the existing carbon should be regenerated. On a Vanta analyzer, calcium can also be analyzed at the same time as measuring gold, silver, and copper.

Portable XRF Analyzers for Measuring Gold in Activated Carbon

Portable XRF vs. Lab Results

The following graphs compare Vanta analyzer versus laboratory results for Au in activated carbon from various minesites and from certified reference materials. The results demonstrate excellent correlation and accuracy between lab and pXRF results. The results also demonstrate the pXRFs ability to monitor trends in Au adsorption within carbon at any minesite and provide support for mineral processing decisions and laboratory operations.

Portable XRF Analyzers for Measuring Gold in Activated Carbon

Portable XRF Analyzers for Measuring Gold in Activated Carbon

Sample Au ppm (Laboratory) Au ppm (Olympus pXRF)
1 544 536
2 784 814
3 1350 1296
4 2370 2387
5 468 477
6 395 443
7 239 299
8 1580 1713
9 1688 1532
10 547 527
11 260 205
12 64 60
GBC314-2 96 119
GBC913-2 508 654
GLC915-3 1472 1673
GLC615-4 3405 3622
GLC615-7 6815 6652
GLC910-3 8713 8698
Plant Cell 2A 9178 8933
Plant Cell 2B 6428 6497
Plant Cell 3A 5666 5845
Plant Cell 4A 2828 3027
Stage 1A 1015 837
Stage 2A 700 700
Stage 3A 390 323
Stage 6A 86 34
Stage 6B 48 26.5

Portable XRF has been demonstrated to be an effective tool to monitor loading trends for gold in activated carbon. The Vanta analyzer’s results are very close to the laboratory results. Real-time monitoring made possible by pXRF can help maintain optimal carbon efficiency and reduce the costs and delays associated with lab analysis.

Olympus IMS

Products used for this application


Vanta for Mining & Geochemistry

Vanta handheld XRF analyzers for mining and geochemistry provide immediate on-site elemental analysis for geochemical exploration, mining grade control, ore processing, and remediation.

DELTA Mining and Geochemistry Handheld XRF Analyzer

DELTA Mining and Geochemistry Handheld XRF Analyzers provide immediate results to help determine the next course of action for the entire process – exploration, ore grade/process control, environmental sustainability. On-site detection of metals, minerals and contaminants. GPS-GIS-XRF for instant metal mapping, time, cost savings.
Sorry, this page is not available in your country

Let us know what you're looking for by filling out the form below.

This site uses cookies to enhance performance, analyze traffic, and for ads measurement purposes. If you do not change your web settings, cookies will continue to be used on this website. To learn more about how we use cookies on this website, and how you can restrict our use of cookies, please review our Cookie Policy.

OK