Ultrasonic time-of-flight-diffraction (TOFD) examination of butt-fusion joints of high-density polyethylene (HDPE)

Background

High-density polyethylene (HDPE) piping has been used in place of steels in the petrochemical, power, and mining industries due to its exceptional resistance to corrosion and erosion. Recently, HDPE has also been used for nuclear safety-related cooling water applications. The application of nuclear quality assurance requirements requires reasonable assurance that the production fusion joint is sound. Ultrasonic time-of-flight-diffraction (TOFD) inspection of fusion joints is an easily employed nondestructive examination tool that can be used to provide additional assurance of fusion-joint integrity.

Problem

The HDPE joint process is typically subject to the following flaws: lack-of-fusion, cold fusion (partial bond), inclusions (embedded), and voids. There is currently no consensus in the industry as to the nature and size of rejectable flaws; however, nondestructive examination is often requested to detect these conditions.

HDPE material has some specific characteristics that make its inspection difficult. Its acoustic impedance and sound velocity is similar to the materials commonly used in ultrasound wedges, which makes it difficult to achieve appropriate refraction of sound at the interface. In addition, coupling between the Rexolite wedges and the material can be difficult to achieve. Also, HDPE material is very attenuative as compared with metals, which often prohibits the use of higher ultrasonic frequencies. It also exhibits a natural high-frequency filtering effect. To overcome these hurdles, low-frequency probes mounted on TOFD Water Wedges are used.

Cross section of an HDPE fusion joint
Cross section of an HDPE fusion joint

Equipment

The following equipment is used for the inspection:

  • OmniScan MXU UT 2 Channel Instrument (or other TOFD-enabled MX unit)
  • Panametrics Preamplifier Model 5682 (500 kHz-30 MHz/30 dB)
  • Panametrics C542-SM or C546-SM Centrascan (6.25 mm or 0.246 in. element dia.; 2.25 MHz and 3.5 MHz frequencies)
  • TOFD (ST1) 60L Water Wedges
  • 1 Chainscan Semi-automatic Scanner (X or XY version)
  • 1 CFU-03 or comparable water delivery system

OmniScan MXU inspection set up
Inspection setup
water wedge water wedge water wedge
Water Wedges

Typical procedure

A conventional TOFD procedure is used for the inspection of HDPE, with the following specifications:

  • The probe centering spacing (PCS) is adjusted to provide beam cross at 66% of the thickness. Additional configurations are recommended on thick-wall pipes to improve detection near the OD or ID surfaces.
  • The probe assembly is mounted on the Chain scanner.
  • Electronic gain on the OmniScan is adjusted to set the lateral wave (LW) signal at 60%.
  • The Chainscan is mounted on the pipe, and the inspection is performed in one rotation.

TOFD (time-of-flight diffraction) pattern of butt-fusion joint HDPE

Time-of-flight diffraction pattern of butt-fusion joint HDPE

Results

The screen capture below, with A-scan and circumferential B-scan images, shows the results on a 25 mm (1 in.) thick HDPE sample with ID calibration cuts ranging in depth from 11.6 mm (0.456 in.) to 2.9 mm (0.114 in.). The three inserted cuts are detected clearly with a good signal-to-noise ratio.

A-Scan screen

The following screen capture clearly shows the presence of voids and/or contaminants in the16 mm (0.629 in.) -thick HDPE butt-joint of a 150 mm (5.9 in.) diameter pipe.

Presence of voids on HDPTE butt-joint

This image is indicative of a poor bonding condition at the inner wall through almost the entire diameter of a 54-mm (2.125 in.) -thick HDPE butt-joint of a 450 mm (17.716 in.) diameter pipe.

Poor Bonding Image

Conclusion

Use of TOFD in conjunction with the OmniScan and other appropriate tools has shown to be a valid method for nondestructive inspection of HDPE butt-fusion joints. While the nuclear industry continues to evolve with respect to detecting rejectable flaws, further studies and trials continue with the use of ultrasound phased array.

Products used for this application

5682

The 5682 ultrasonic preamplifier provides low noise 30 dB amplification of ultrasonic signals ranging from 500 KHz to 25 MHz. The preamplifier, housed in a rugged splash-proof enclosure, is very small and lightweight making it ideally suited for remote applications.

CFU Couplant Feed Unit

The CFU-03 and CFU-05 are portable electric pump units used to supply constant couplant flow to wedges during ultrasonic inspections.

CHAIN Scanner

The CHAIN scanner provides a manual pipe-inspection solution for pipes between 1.75 to 38 in. OD. The scanner, held by chain links instead of magnetic wheels is well suited for weld or corrosion inspection on different type of materials. UT, TOFD, PA.

OmniScan MX UT

The OmniScan MX UT performs conventional UT and automated inspections and supports TOFD as well as encoded B-scan and C-scan, and full data storage. Allows inspections that simultaneously combine TOFD with conventional pulse echo.

TOFD Transducers & Wedges

TOFD transducers and wedges generate refracted longitudinal waves in steel for use in applications involving crack sizing by means of the Time of Flight Diffraction technique.

Ultrasonic Transducers

Ultrasonic transducers are used for applications as diverse as flaw detection, thickness gaging, materials research and medical diagnostics. More than 5000 ultrasonic transducer types come in many styles, element diameters, frequencies, and connector styles.

Inspection & Measurement Systems
English | 日本語 | français | 简体中文 | Deutsch | italiano | čeština | magyar | Tiểng Việt | Español | русский | polski | português | 한국어

Advanced NDT Solutions

Flaw Detectors

Integrated Inspection Systems