Background

Transmit-Receive Longitudinal (TRL) conventional probes are advantageously used for the inspection of dissimilar metal welds and other acoustically noisy material. Dual matrix array (DMA) probes combine the advantages of TRL probes with the advantages of phased-array technology allowing electronic steering, skewing and focusing of acoustic beams.

Problematic

Dissimilar and austenitic welds are very difficult to inspect with ultrasound, especially when the inspection has to be done from only one side since the ultrasonic beam is scattered due to the anisotropy of the weld material.

A TRL is basically a dual element probe with one emitter and one receiver separated by acoustic insulation. The squint and roof angles configuration allows focusing at one point in the part and creates a pseudo-focalization. These probes eliminate the interface echo, have no dead zones due to wedge echoes, reduce the backscattering signals and permit the use of higher gain.

As a TRL probe has a fixed refracted angle and pseudo-focal point, a typical inspection can require many of these probes to cover a range of different configurations.

Solutions

Dual matrix arrays (DMA) are the logical evolution of this technology. Composed of two matrix arrays, the beam can typically be swept from 30 to 70 degrees (LW or SW), the pseudo-focal point can be adjusted at different depths, the beam size can vary by selecting different aperture sizes and the beam can be skewed looking for oblique defects. Used in conjunction with an OmniScan MX and its imaging, a dual matrix array is more flexible that a TRL probe as it can adapt to different configurations electronically.

Equipment

The equipment used for the inspection is comprised of:

Portable phased-array equipment:

OmniScan MX or MX2 32/128 PR Module
1 dual matrix array: 1.5DM7X4-19X12-A17-P-2.5-OM-DUAL28
1 flat wedge SMA17-DN50L5

phased array probes

Pictures of the dual matrix array mounted on a wedge

Dual matrix array schematic representation

The dual matrix array used is the 1.5DM7X4-19X12-A17-P-2.5-OM-DUAL28 mounted on a wedge. Full apertures of 28 elements were used at the emission and reception using the full active surface of 19 mm x 12 mm (each matrix).

The OmniScan MX 32: 128 PR was programmed with 3 different sectors with beam steering from 30° to 70° LW for each of them but with different skew angles of -15°, 0° and 15°. All beams were set to focus at the ID of the pipe.

Results

The picture below shows the results on a pipe-to-pipe stainless steel weld. The dual matrix array was programmed with a sector scan from 30° to 70° LW and a skew of 0°. An ID connected crack of 1.1 (long) in x .3 in (height) is clearly detected.

A-scan screen from OmniScan

The picture below shows the results on a pipe-to-pipe stainless steel weld. The dual matrix array was programmed with a sector scan from 30° to 70° LW with 3 different skew angles (-15, 0 and 15 degrees). In this case, an ID connected crack of 1.5 (long) in x .4 in (height) is better detected with a skew angle of -15 degrees. In this configuration, even the crack tip is visible.

Multiple A-scan screens from OmniScan

Conclusion

Dual matrix arrays can be advantageously used during the inspection of noisy material. When used with a portable phased-array instrument like the OmniScan, these probes are more flexible than conventional TRL probes.

Products used for this application

OmniScan MX

The OmniScan MX is an advanced, multi-technology flaw detector. It offers a high acquisition rate and powerful software features-in a portable, modular instrument to efficiently perform manual and automated inspections. Available with PA and conventional UT modules, and conventional EC and ECA modules.

OmniScan MX PA

The OmniScan PA performs manual and automated phased array inspections. It offers full-featured A-scan, B-scan, S-scan and C-scan displays, and advanced real-time data processing. Configurable in 16:128 elements, also 16:16M, 16:64M, 32:32, and 32:128

OmniScan MX2NEW

The OmniScan MX2 phased array flaw detector with touch screen interface offers increased testing efficiencies and powerful software features, ensuring superior manual and advanced AUT application performance with fast setups, test cycles, and reporting. It is compatible with all existing phased array modules.

Inspection & Measurement Systems
English | 日本語 | français | 简体中文 | Deutsch | italiano | čeština | magyar | Tiểng Việt | Español | русский | polski | português | 한국어

Advanced NDT Solutions

Flaw Detectors

Integrated Inspection Systems