Recommended instruments:
Background: The very high temperatures found inside steam boilers (in excess of 1500 degrees Fahrenheit or 800 degrees Celsius) can cause the formation of a specific type of hard, brittle iron oxide called magnetite on the inside and outside surfaces of steel boiler tubing. The presence of this oxide layer on the outside of tubes can interfere with ultrasonic wall thickness measurement using common dual element transducers, both because it can have a very rough surface that prevents proper sound coupling, and because oxide thickness will be added to the steel thickness. However, as its name implies, magnetite is magnetic, and that property permits the use of magnetostrictive EMAT (Electomagnetic Acoustic Transducer) transducers such as the Panametrics-NDT E110-SB. EMATs offer several advantages over conventional dual element piezoelectric transducers: it is not necessary to remove oxide scale in order to make measurements, the scale thickness is not added into the wall thickness measurement, and measurements can be made very quickly and without need for liquid couplant. The primary limitation of magnetostructive EMATs is that they work only when scale is present and bonded to the outside of the boiler tube. Additionally, the minimum measurable wall thickness and measurement accuracy will not be nearly as good as what can be achieved with a conventional dual, and EMATs are relatively insensitive to small internal pits. For that reason, EMATs are often used for quick initial wall thickness surveys, while duals can then be used to take a closer look at areas of concern. Theory of operation: There are two types of EMATs used within the NDT industry. One is known as a Lorentz EMAT, which does not require the presence of oxide scale, but does require very high driving power. A magnetostrictive EMAT such as the E110-SB requires scale but works at the much lower power levels typical of field portable ultrasonic gages and flaw detectors. It consists of a strong permanent magnet and a coil which acts as an electromagnet when driven by the excitation pulse from the test instrument, as seen in Figure 1. The permanent magnet creates a magnetic field perpendicular to the surface of the scale (Bs in the figure below), while the dynamic field created by the electromagnet (B d) causes the scale to be pulled radially outward and inward as the coil is pulsed, as seen in Figure 2. This motion generates a normal incidence shear wave in the scale, which then propagates into the steel. Essentially, the scale acts as the active transducer element to generate the sound pulse. The frequency of the sound pulse will vary as oxide thickness changes, increasing as oxide becomes thinner and decreasing as oxide becomes thicker. With typically thin scale buildups, the frequency will be approximately 5 MHz. The process also works in reverse to generate a voltage in the coil when the returning shear wave echo vibrates the scale.
Because the scale itself is the transducer element, scale roughness is not a coupling issue, and the scale is not added into the thickness measurement. The EMAT generates a shear wave, so the instrument must be calibrated to a shear wave velocity of approximately 0.1280 in/uS or 3,240 m/S in typical carbon steel. Typical measurement accuracy with the E110-SB EMAT transducer will be +/- 0.010 inch or 0.25 mm, with a minimum
measurable thickness of at least 0.080 in. or 2.0 mm depending on material properties.
|
The EPOCH 600 is mid-level, handheld ultrasonic flaw detector. Weighing only 1.68 kg (3.72 lb.), its horizontal case is built to withstand the rigors of very harsh environments. EN12668-1 plus features such as 400 V PerfectSquare tunable square wave pulser, digital filtering for enhanced signal-to-noise ratio.Copyright 2011 OLYMPUS CORPORATION, All rights reserved. Terms Of Use | Privacy Statement